Comparable Specifications and Designations

View Typical Chemical Composition
Alloy TypeRolls-RoyceSnecmaGEHoneywellOthers
17/4PH-----
JetheteMSRR6643----
Maraging Steel----NGMS 800
N155----Multimet

Typical Chemical Composition - wt %*

View Comparable Specifications and Designations
Alloy TypeAlBCNbCoCrFeMnMoNiSiTaTiWZROthers
17/4PH--0.04--16.0Bal0.04-4.00.70----Cu 3.20, Nb+Ta 0.25
Jethete----1.511.7Bal-1.72.8-----V 0.3, N 0.03
Maraging Steel----10.3-Bal-4.716.8--0.3---
N155----19.521.0Bal-3.020.0---2.5-N 0.14

Comparable Specifications and Designations

View Typical Chemical Composition
Alloy TypeRolls-RoyceSnecmaGEHoneywellOthers
AIRESIST 319---EMS 55455-
B1900----PWA1402, MTS1083
B1914-----
C1023MSRR7046----
C130MSRR7045----
C242MSRR7217----
C263MSRR7040DMD442-32---
CHS70-----
CHS88-----
CHS104-----
CNK7-----
GMR235-----
GDT111--B50A719--
GTD111DS--B50A858--
GTD222--B50A850--
GTD241--B50A972--
GTD262--B50A985--
GTD741--B50A973--
Alloy XMSRR721----
Haynes 230™MSRR7269---PWA1474
Haynes 282™-----
IN100MSRR7047DMD432-32C5OTF107 EMS55425PWA658
IN600-----
IN625MSRR7198-B50TF107EMS55425PWA1465
IN713CMSRR7164DMD421.22B50TF16EMS55371PWA655, PWA649
IN713LCMSRR7048-B50TI239EMS55079-
IN718MSRR7132DMD423.32C5TF89EMS55458PWA649, PWA1451
IN718SQMSRR7228----
IN738CMSRR7133, 7125-B50A563A-PWA1451
IN738LCMSRR7168, 7173-B50A563BEMS55445-
IN792-5AMSRR7169, 7239----
IN939----MTS1348, HXLM00424
MM002MSRR7101, 7080, 7150----
MM246MSRR7061, 7062----
MM247---EMS55447MTS1206
M247LC-----
MM421----M3612
N75MSRR7004----
N80NSRR1077----
N90MSRR1789----
PE10MSRR7184---PWA1056
PWA1056----PWA1056
PWA1188----PWA1188
PWA1422----PWA1422
PWA1432----PWA1432
PWA1437----PWA1437
PWA1440 (SC)----PWA1440
PWA1455----PWA1455
PWA1467----PWA1467
PWA1475----PWA1475
PWA1480 (SC)----PWA1480
PWA1483----PWA1483
PWA1484 (SC)----PWA1484
Rene 41--B50TF37--
Rene 77-DMD437.32C50TF15--
Rene 80--C50TF47-PWA1449
Rene 108----B50TF262
Rene 125--C50TF60--
Rene 142--C50TF94--
Rene 220--C50TF91--
Rene N2--C50TF121--
Rene N4--C50TF75--
Rene N5--C50TF122--
Rene N6--C50TF114--
Rene N500--C50TF129--
Rene N515--C50TF130--
SX-4-----
SRR99MSRR7210---MTS1162
RR2000MSRR7225----
U500--B50A467--
U700--B50A524-PWA656
WASPALOY----PWA1471

Typical Chemical Composition - wt %*

View Comparable Specifications and Designations
Alloy TypeAlBCNbCoCrFeMnMoNiSiTaTiWZROthers
AIRESIST 3195.300.0100.182.0-13.0--4.2Bal--0.8-0.07-
B19006.000.0150.10-10.08.0--6.0Bal-4.31.0-0.07-
B19145.500.100--10.010.0--3.0Bal--5.3---
C10234.100.0060.15-9.715.5--8.0Bal--3.6---
C1300.85-0.06--21.5--9.8Bal--2.6---
C2420.15-0.31-10.021.0-0.3510.5Bal0.35-0.2---
C2630.50-0.06-20.020.0--5.8Bal--2.2---
CHS703.00-0.090.210.515.5--1.9Bal--4.55.20.02-
CHS883.400.0800.070.110.515.9--1.9Bal--4.65.3-Hf 0.30
CHS1042.500.0130.110.311.021.0--0.6Bal--3.53.5--
CNK73.400.0120.12-4.513.2--0.7Bal--4.77.0--
GMR2353.600.0500.15--15.510.000.305.0Bal0.40-2.0---
GDT1113.000.0100.10-9.514.0--1.5Bal-2.84.93.80.01-
GTD111DS3.000.0100.10-9.514.0--1.5Bal-2.84.93.8<0.01-
GTD2221.200.0100.100.819.022.5---Bal-1.02.32.00.02-
GTD2411.200.0040.10-19.022.5---Bal--2.32.00.01Nb+0.508Ta 1.3
GTD2621.700.0060.01-19.022.5---Bal--2.32.00.01Nb+0.508Ta 1.35
GTD7413.500.0120.10-8.516.0--1.8Bal--3.52.60.02Nb+0.508Ta 1.8
Alloy X-0.8000.08-22.018.5-0.508.5Bal0.08--0.6--
Haynes 230™0.350.0050.07--22.0-0.602.0Bal0.45--14.0--
Haynes 282™1.550.0060.06-10.020.51.50-8.5Bal--2.1---
IN1005.500.0150.17-15.09.7--3.0Bal--4.7-0.04V 0.9
IN600--0.10--15.58.000.80-Bal0.30-----
IN6250.20-0.053.6-21.53.000.209.0Bal0.20-0.2---
IN713C6.000.0100.152.2-13.5<2.00-4.2Bal--0.8-0.07-
IN713LC6.000.0100.062.0-12.0--4.2Bal--0.8---
IN7180.60-0.06--19.0Bal-3.052.5--0.9--Cb+Ta 5.0
IN718SQ0.60-0.06--19.0Bal-3.052.5--0.9--Cb+Ta 5.0
IN738C3.400.0100.170.88.416.0--1.7Bal-1.83.42.60.06-
IN738LC3.400.0100.100.88.416.0--1.7Bal-1.83.42.60.03-
IN792-5A3.400.0150.08-9.012.6--2.0Bal-4.04.04.00.03-
IN9391.900.0100.151.019.022.5---Bal-1.43.72.00.09-
MM0025.500.0150.15-10.09.0---Bal-2.51.510.00.04Hf 1.4
MM2465.500.0150.15-10.09.0--2.5Bal-1.51.510.00.05-
MM2475.500.0150.15-10.08.4--0.7Bal-3.11.010.00.04Hf 1.4
M247LC5.600.0150.07-9.38.1--0.5Bal-3.20.79.500.1Hf 1.4
MM4214.200.0150.151.810.015.8--2.0Bal------
N750.20-0.12--19.5-0.60-Bal0.60-0.4---
N801.20-0.07--20.0-0.60-Bal0.60-2.6---
N901.20-0.09-16.020.0-0.60-Bal0.60-2.6---
PE10--0.046.7-20.03.000.306.0Bal0.25--2.5--
PWA 1056---------Bal------
PWA 11883.400.0250.050.920.313.0--3.8Bal-2.43.72.10.05-
PWA 14225.000.0150.141.010.09.0---Bal--2.012.0-1.6Hf
PWA 14323.500.0120.11-9.012.2--1.9Bal-5.04.13.80.004-
PWA 14373.600.0120.11-9.012.1--1.9Bal-5.04.13.8<0.02-
PWA 1440 (SC)5.000.003/mx0.04-5.010.0---Bal-12.01.54.00.03/mxHf 0.35
PWA 14556.000.0150.10-10.08.0--6.0Bal-4.31.0-0.04Hf 1.1
PWA 14673.400.0150.12-9.012.4--2.1Bal-4.24.04.00.06Hf 0.5
PWA 14756.600.0070.10--10.0--2.0Bal-4.1-3.20.3Hf 1.2
PWA 1480 (SC)5.000.003/mx0.05/mx-5.010.0---Bal-12.01.54.00.015/mx-
PWA 14833.600.003/mx0.07-9.012.2--1.9Bal-5.04.13.80.0075/mx-
PWA 1484 (SC)5.600.003/mx0.05/mx-10.05.0--1.9Bal-8.7-6.00.015/mxRe 3.0 Hf 0.1
R411.650.0060.09-11.019.0--9.5Bal--3.1---
R774.300.0150.07-15.014.7--4.2Bal--3.4-0.04-
R803.000.0150.17-9.414.0--4.0Bal--5.04.00.02-
R1085.500.0150.08-9.58.4--0.5Bal-3.00.89.50.01Hf 1.5
R1254.800.0150.11-10.08.9--2.0Bal-3.82.47.00.04Hf 1.6
R1426.100.0150.12-11.86.8--1.5Bal-6.40.02/mx4.90.03/mxHf 1.5 Re 3.0
R2200.500.0040.035.312.019.0--3.2Bal-3.31.0---
N26.600.0040.04-7.513.0---Bal0.055.00.04/mx3.80.015/mxHf 0.1 Re 1.6
N44.200.0040.060.57.59.8--1.5Bal-4.83.56.0-Hf 0.15
N56.200.0040.05-7.57.0--1.5Bal-6.50.04/mx5.0-Hf 0.15 Re 3.0
N65.800.0040.05-12.54.2--1.4Bal-7.20.04/mx6.0-Hf 0.15 Re 5.4
N5006.600.0040.04-7.56.0--1.5Bal-6.60.04/mx6.3-Hf 0.15
N5156.300.0040.05-7.56.0--2.0Bal-6.50.04/mx6.3-Hf 0.6 Re 1.5
SX-45.60-0.006/mx-9.66.4--0.6Bal-6.51.06.4-Hf 0.09 Re 2.95
SR995.50-0.02-5.18.5---Bal-2.82.29.4--
RR20005.50-0.015-15.010.0--3.0Bal--4.0--V 1.0
U5003.000.0080.08-17.519.0--4.0Bal--2.9---
U7004.300.0200.80-15.015.0--4.5Bal--3.3---
WASPALOY1.100.0050.07-13.519.5--4.3Bal-3.0--0.07-

Comparable Specifications and Designations

View Typical Chemical Composition
Alloy TypeRolls-RoyceSnecmaGEHoneywellOthers
CoCrMo----HS21, ASTM F75
ECY768----HS21, ASTM F75
FSX414--B50A910--
X40MSRR7049, 7122DMD403.32C50TF21-HS31, PWA648
X45-DMD405.32B50A3744B--
MM302----PWA657
MM509-DMD.401-32B50TF89EMS55451PWA647

Typical Chemical Composition - wt %*

View Comparable Specifications and Designations
Alloy TypeAlBCNbCoCrFeMnMoNiSiTaTiWZROthers
CoCrMo--0.23-Bal28.0-0.506.0-0.80-----
ECY7680.20-0.60-Bal23.5---10.0-3.50.27.0--
FSX414-0.1000.25-Bal29.5-0.70-11.00.90--7.0--
X40--0.50-Bal25.5-0.80-10.50.80--7.5--
X45-0.1000.25-Bal25.5-0.50-10.50.80--7.5--
MM302-0.0050.85-Bal21.5-----9.0-10.00.02-
MM509--0.60-Bal23.5---10.0-3.50.27.00.45-